3+ 11
Erbium (Er , 4f )— continued
Host Laser Wavelength Temp. Optical
crystal transition ( m) (K) pump Mode Ref.
4
LiYF :Pr 4 S 3/2 fi I 13/2 0.8503 110, 300 Xe lamp p 224, 329
4
4
LiYF :Pr 4 I 11/2 fi I 13/2 »2.8 300 laser diode cw 1070
4
4
LiYF :Tb 4 S 3/2 fi I 13/2 0.8503 110, 300 Xe lamp p 224
4
4
LiYF :Yb 4 S 3/2 fi I 15/2 0.551 300 TiS laser upc 1030
4
4
4 S 3/2 fi I 11/2 1.234 300 TiS laser cw 734
4
4 F 9/2 fi I 11/2 2.0025 300 NdYLF p, upc 813
4
LiY 0.5 Er 0.5 4 4 S 3/2 fi I 13/2 0.8501 113, 161 Xe lamp p 181
F
0.8535 113, 163 Xe lamp p 181
4
LuAlO 3 4 S 3/2 fi I 9/2 1.6675 90 Xe lamp p 795
4
LuAlO :Tm 4 I 11/2 fi I 13/2 2.7126 ~110 Xe lamp p 792
3
4
Lu Al O 12 4 S 3/2 fi I 13/2 0.8631 110 Xe lamp p 218
5
3
0.86325 77, 300 Xe lamp p 239
4
4 I 13/2 fi I 15/2 1.6525 77 Xe lamp p 794
1.6630 77 Xe lamp p 794
4
4 S 3/2 fi I 9/2 1.7762 300 Xe lamp p 790
4
Lu Al O 12 4 I 11/2 fi I 13/2 2.7973 300 Xe lamp p 918
5
3
2.7998 110 Xe lamp p 918
2.829 300 ErGL p, upc 1094
2.8297–2.8302300 Xe lamp p 918
2.8552–2.8590110 Xe lamp p 918
2.8700 110 Xe lamp p 918
2.8748–2.8752110 Xe lamp p 918
2.8760 110 Xe lamp p 918
2.8967–2.8979110 Xe lamp p 918
2.9395 300 Xe lamp p 239
2.9395–2.9397110 Xe lamp p 918
2.940 300 ErGL p, upc 1094
2.9401 110 Xe lamp p 918
2.9408 300 Xe lamp p 239
4
Lu Al O : 4 I 11/2 fi I 13/2 2.6990 300 Xe lamp p 239
12
5
3
Ho,Tm
4
Lu Al O : 4 I 11/2 fi I 13/2 2.8298 300 Xe lamp p 941
5
12
3
Cr,Yb 2.9395 300 Xe lamp p 239
2.9405 300 Xe lamp p 941
4
(Lu,Er) Al O 12 4 S 3/2 fi I 13/2 0.8625 300 Xe lamp p 218
3
5
4
4 S 3/2 fi I 13/2 0.8631 110 Xe lamp p 218
4 S 3/2 fi I 9/2 1.7767 110 Xe lamp p 790
4
4
4 I 11/2 fi I 13/2 2.6990 300 — — 239
©2001 CRC Press LLC