30.3 Flash Troubleshooting  291

































          Figure 30.7  Calculate required cylinder size



          30.3.2.7„ Mold: Mismatch
          Sometimes what is being called flash is actually a mismatch in the parting line. No
          matter what is changed on the machine or the process a mismatch will not im-
          prove. shows an example of a mismatched parting line. When feeling for parting
          line flash, true flash can be felt from both directions across the parting line, but a
          mismatch will only be felt from one direction.

          A mismatched parting line can arise from excessive polishing along the parting
          line. Removing too much steel from one side of the mold during polishing can cre-
          ate a mismatch that is objectionable. Care must be exercised when polishing near
          a parting line.


















          Figure 30.8  Mismatched parting line