Density  (g/cm 3 )  2.34 2.50  2.48 2.56  2.46 2.97  2.3 2.4




                 Elastic  modulus  (GPa)  42 48     30 40     2015.


                 Compressive  strength  (MPa)  30 70  38 42  45 70  40 57.5  al.,  et Takahiro  2017.  al., Santamarıa et  ´





                   (cm)                           2017;  al.,  et  2018;
                 Abrams  slump  7 20  7.6  15 20  SCC  Cheng  2017;  al., Santamarıa et  ´





                 Admixture  (Type,  cement)  %  Superplasticiser  1.18%     Superplasticiser,  1 2%  1.3 2.5  Bai,  and Dadsetan  2018;  al.,  et



             aggregate   0.56 1.2  0.5 0.56  0.5 0.7  0.46 0.6  2018;  al.,  Ortega-Lopez  ´



             as  Water/  cement  ratio            et  Majhi
             slags                              furnace.  1933;  2009;

             using  Cement  (kg/m 3 )  156 357  243 386  300 400  300 370  LF, Ladle  MSHL,  Gaddo,  and

             performed  (mm)  11 20  12.5 22  ,0.1  furnace;  arc  Laboratory  Pellegrino



             concrete  Slag  size  2 19   Filler  Electric  Highway  2013;  al.,  et


             of                structural  structural,  compacting  compacting  EAF,  State  Pellegrino
             types  Concrete  type  Structural  Plain,  Plain,  self-  Self-  furnace;  Michigan  2015.

             main                               oxygen  2012;  Singla,  2015;  2015.
             of                                 Basic  and  Sharma  Roesler,  al.,  et
             Characteristics                    BOF,  slags;  Transportation,  of  2015;  and  Brand  Sideris  2014;






             7.2                                Air-cooled  Department  Roesler,  and  2017;  Sosa,  al.,  et
             Table  Slag  ABS a  BOF b  EAF c  LF d  ABS,  a US  b Brand  c Israel  d Anastasiou
   204   205   206   207   208   209   210   211   212   213   214