GPC100RA  0  414  515  0  956  0  69  138  8.3  0.5







                         2016)  GPC75RA


                         Kaliyaperumal,  0  414  515  239  717  0  69  138  8.3  0.5





                         and  GPC50RA
                         (Kathirvel  0  414  515  478  478  0  69  138  8.3  0.5



                         concrete  GPC25RA


                         geopolymer  0  414  515  717  239  0  69  138  8.3  0.5




                         on
                         based  GPC0RA

                         RCA    0  414  515  956  0  0  69  138  8.3  0.5
                         with

                         AASc  OPC  414  0  515  956  0  207  69  0  0  0.5

                         of
                         mixes

                         of            (kg/m 3 )  (kg/m 3 )
                         Composition   aggregates  aggregates  (kg/m 3 )  (kg/m 3 )  solution  (kg/m 3 )  ratio





                         13.6   (kg/m 3 )  (kg/m 3 )  (kg/m 3 )  (kg/m 3 )  solution  Superplasticizer  Liquid/binder
                         Table  Label  Cement  GGBFS  Sand  Natural  Recycled  Water  NaOH  Na 2 SiO 3