Page 235 - Lindens Handbook of Batteries
P. 235

ZINC-CARBON BATTERIES—LECLANCHÉ AND ZINC CHLORIDE CELL SYSTEMS       9.29

                                               TABLE 9.6  Flash Current and Internal Resistance for Various
                                               Battery Sizes

                                                         Typical maximum flash  Approximate internal
                                                              current, A    resistance, ohms
                                                  Size      LC*     ZC*      LC     ZC
                                               N            2.5      ...    0.6      ...
                                               AAA          3       4       0.4     0.35
                                               AA           4       5       0.30    0.28
                                               C            5       7       0.39    0.23
                                               D            6       9       0.27    0.18
                                               F            9       11      0.17    0.13
                                               9 V (battery)  0.6   0.8     5       4.5
                                                 *LC: Leclanché, ZC: Zinc chloride.
                                                 Source:  Eveready Battery Engineering Data. 12




















                                     FIGURE 9.28  Comparison of voltage and internal resistance during discharge of a 9 V battery on
                                     smoke detector test. Background load = 620,000 ohms continuous; pulse load = 1,500 ohms × 10 ms
                                     every 40 s.


                                   The  internal  resistance  of  zinc-carbon  batteries  increases  with  the  depth  of  discharge.  Some
                                applications use this feature to establish low-battery alarms to predict near end of battery life situa-
                                tions (such as in the smoke detector). Figure 9.28 shows the relative battery internal resistance versus
                                depth of discharge of a 9 V Leclanché battery.
                                   One of the reasons for this increase in internal resistance is the cathode discharge reaction. The
                                porous cathode becomes progressively blocked with reaction products. In the case of the Leclanché
                                system, it is in the form of diammine-zinc chloride crystals; in the case of the zinc chloride system, it is
                                in the form of zinc oxychloride crystals. Also the conductivity of the manganese dioxide decreases.


                    9.6.7  Effect of Temperature

                                Zinc-carbon batteries operate best in a temperature range of 20 to 30°C. The energy output of the
                                battery increases with higher operating temperatures, but prolonged exposure to high temperatures
                                (50°C and higher) will cause rapid deterioration. The capacity of the Leclanché battery falls off rap-
                                idly with decreasing temperatures, yielding no more than about 65% capacity at 0°C, and is essentially
                                inoperative below -20°C. Zinc chloride batteries provide an additional 15% capacity at 0°C or 80%
   230   231   232   233   234   235   236   237   238   239   240